Abstract

Surfaces of plated tin-lead deposits dulled by dark oxides can be cleansed and brightened by immersion, for 3-5 minutes, in the solution: Na Cl O(2) - 6 pbw Na(3) PO(4) - 1 pbw Na OH - 0.5 pbw Dl water - 100 pbw Operating Temperature: 200 degrees F.

This text was extracted from a PDF file.
This is the abbreviated version, containing approximately 100% of the total text.

Page 1 of 1

Brightener for Plated Tin Lead Surfaces

Surfaces of plated tin-lead deposits dulled by dark oxides can be cleansed and brightened by immersion, for 3-5 minutes, in the solution: Na Cl O(2) - 6 pbw

Na(3) PO(4) - 1 pbw

Na OH - 0.5 pbw

Dl water - 100 pbw

Operating Temperature: 200 degrees F.